Tacked my tube sheet from the middle out last turnaround and the warpage dropped to almost nothing
I've always started my tack welds at the edges and worked toward the center, mostly because that's how the guy who trained me in Beaumont did it back in 2009. Last month on a heat exchanger job I decided to flip it and tack the middle first, then work outward in a cross pattern about 6 inches apart. The tube sheet came out with less than 1/16 inch of bow across the whole face, where I used to fight 3/16 or worse and end up reaming holes to get tubes to slide. I also let each tack cool for a minute before moving to the next one instead of chasing the heat around. Maybe it was the plate, maybe it was dumb luck, but I'm going to run it the same way on the next one to see if it holds up. Curious if any of you have run the center-out pattern on bigger tube sheets and whether the relief cuts matter as much as I think they do.