Question about a pour in Gary that went sideways in 20 minutes
Two weeks ago we did a 40x60 slab for a guy's shop out near Gary. Mud came in hot, 6 inch slump, no water added on site that I saw. We got it struck off and started floating and the surface started tearing bad on the west half where the sun hit first. Lead guy hollered to get the trowels off it and cover it with burlap, wet it down, and just wait. Killed about 45 minutes. Then it finished clean as anything, no blisters, no dust. I still don't get why the tearing stopped so fast. Was it the wind drying the top or was that batch just hotter than the rest? What do you check first when the finish starts fighting you?
Did you check the mix temp before it left the plant? I used to blame wind every time, but once I started watching batch temps I learned the hot loads tear way sooner, and shade plus burlap buys you just enough time to finish clean.